Ir para o conteúdo principal Saltar para a pesquisa Saltar para a navegação principal
Experiência em inúmeros projetos
Vamos começar juntos
Somos diferentes. Somos melhores!
Contacto rápido e direto
Oferta
Ir para a página inicial

X-Ray and CT Inspection of Die Castings: Methods, Standards and Limits

FISS Knowledge title graphic on X-ray and CT inspection of die castings with a YXLON MU 2000 X-ray inspection system and its control desk
FISS Knowledge · Quality Inspection

X-Ray and CT Inspection of Die Castings: Methods, Standards and Limits

A die casting can look perfect and still contain pores in a sealing face or a load-bearing rib. X-ray methods make the inside visible without destroying the part. Whether a 2D image in the production cycle or a CT scan in the lab fits depends on the question, the part and the agreed acceptance criteria.

Short Answer

How Are Die Castings Inspected with X-Rays?

X-ray inspection of die castings uses the different absorption of X-rays by sound metal and by voids: pores, shrinkage and inclusions appear as contrast differences. In production, radioscopy with digital detectors delivers real-time 2D images, often with automated defect recognition. Industrial computed tomography (CT) shows position, size and volume of each defect in 3D, but takes much longer per part.

Standards such as ASTM E505 or the BDG guidelines provide a common language for defect types and severity levels. What is acceptable for a specific part is agreed between customer and foundry.

Overview

Three Methods, Three Typical Uses

Radiation passes through the part, and a detector or film records how much arrives – where metal is missing, more gets through. The methods differ in how the image is captured and whether the result is a projection or a volume.

2D, Real Time

Radioscopy

Live image on a digital detector, part moved by a manipulator. Fast enough for 100% inspection in the cycle.

2D, Static

Film and Digital Radiography

Single exposures on film, imaging plates (CR) or detector arrays (DDA), mainly for sampling and documentation.

3D

Computed Tomography

Many projections reconstructed into a volume: exact defect location and size, plus geometry.

X-ray and CT find internal defects but do not explain them; root causes are covered in Die Casting Defects Explained.

2D Inspection

Radioscopy and Radiography: The 2D View

In radioscopy, the casting is moved between X-ray tube and flat-panel detector, and inspector or software evaluate live images from defined viewing angles. For one of its systems for large structural castings, ZEISS states about 3 to 3.5 seconds per view (manufacturer statement); the time per part depends on the number of views.

Radiography records single images – on film, increasingly on imaging plates or digital detector arrays. For castings, EN 12681-1 covers film and EN 12681-2 digital detectors, aiming at a sensitivity equivalent to film.

A Projection Hides Depth A 2D image adds up everything along the beam path: it shows a void, but not its depth. Overlapping walls, ribs and bores complicate interpretation – a common reason to use CT for critical questions.
Computed Tomography

Industrial CT: Voxel Size, Part Size and Scan Time

In CT, the part rotates while the detector records many projections, which are reconstructed into a volume of voxels. If the whole part must fit into the field of view, the voxel size is roughly the scanned width divided by the number of detector pixels across. Large parts mean coarser voxels – unless only a region of interest is scanned at higher magnification.

Scanned width Approx. voxel size* Typical use
30 mm (sample, cut-out) ≈ 0.01 mm Detailed pore analysis, cut-outs from larger parts
150 mm (housing, bracket) ≈ 0.05 mm Porosity analysis and nominal/actual comparison of complete parts
400 mm (large housing) ≈ 0.13 mm Larger defects, overview scans, first-article inspection

*Illustrative estimate for a detector about 3,000 pixels wide; real values depend on system, scan mode and material. A pore must cover several voxels to be measured reliably, so define the smallest relevant pore size before scanning.

  • Porosity analysis: volume, size, shape and position of each pore per part region
  • Nominal/actual comparison: scan versus CAD model, including inner contours
  • Wall thickness analysis: thin areas and core shift in housings and channels
  • Limitations: scan and evaluation from minutes to hours, artefacts on large parts, high cost
Inspection Strategy

Inline Inspection or Sampling?

The choice depends on part risk and cell cycle time. Many plants combine fast 2D inspection in the line with CT in the lab for process qualification and root-cause analysis.

Criterion Inline / at-line radioscopy Offline sampling (2D or CT)
Coverage Up to 100% of parts, defined zones Selected parts per shift, batch or die change
Evaluation Automated defect recognition (ADR) or operator Inspector, CT evaluation software
Information Pass/fail per view, defect indication Exact defect geometry, trends, root cause
Main limitation Must keep pace with the cell cycle Defects between samples go unnoticed

Automated defect recognition evaluates images against learned or rule-based criteria. It must be taught with real good and bad parts and checked regularly for false calls and slip-through. Linking each result to the shot number allows comparison with shot curves; how sorting and marking fit into the cell is covered in Automation in the Die Casting Cell.

Standards

Which Standards Are Relevant?

These documents are frequently referenced for die castings. Check the current edition before writing one into a drawing or supply agreement.

Document Content Note
ASTM E505 Reference radiographs for aluminium and magnesium die castings: discontinuity categories in four severity levels Current edition E505-22; film only, for digital images ASTM E2973
ASTM E2973 Digital reference images for aluminium and magnesium die castings Current edition E2973-22
EN 12681-1 / -2 Founding – radiographic testing: film techniques (Part 1) and digital detectors (Part 2) Editions 2017; a revision of Part 1 is in preparation
VDG P 201, BDG P 202 Volume deficits (porosity) of non-ferrous castings, evaluated in sections German guidelines, 2D evaluation
BDG P 203 Porosity analysis of Al, Mg and Zn castings with industrial CT Extends P 201/P 202 to 3D, evaluation by part region
ISO 15708 series Radiation methods for computed tomography: terminology, principles, operation, qualification Several parts revised since 2024

ISO 10893 covers steel tubes and is not relevant for die castings.

Acceptance Criteria

Acceptance Criteria Are a Matter of Agreement

Reference radiographs show what a severity level looks like, not which level a part may have; ASTM E505 assumes an agreement between purchaser and manufacturer. A typical approach:

01

Define zones

Mark sealing faces, threads, load-bearing sections and machined surfaces on the drawing.

02

Set limits per zone

Severity level or, for CT, maximum pore size, volume or distance to machined surfaces.

03

Fix method and scope

Agree on method, views or CT resolution, frequency and reference standard.

04

Qualify with real parts

Prove with parts from the production die that the method finds the relevant defects.

If porosity sits near machined surfaces, the fix lies in the process: see Mold Filling and Vacuum in Die Casting and Aluminium Melt Quality.

Limits

Where X-Ray and CT Reach Their Limits

  • Wall thickness and contrast: the thicker the section, the weaker the contrast of a given void.
  • Orientation: thin, flat cracks and cold shuts show mainly when the beam runs along their plane.
  • Resolution: micro-porosity below detector or voxel resolution is missed, even if it affects leak tightness.
  • Surface defects: flow marks and surface laps are better found visually.
  • Cost and time: CT for every part is rarely economical.
Radiation Protection X-ray systems are subject to radiation protection law – in Germany the Strahlenschutzgesetz and Strahlenschutzverordnung. Depending on the system type, operation must be notified to or licensed by the competent authority, often with a qualified radiation protection officer. Clarify this with authority and supplier before installation.
Conclusion

Choose the Method to Fit the Question

Radioscopy with automated evaluation inspects many parts inline, radiography documents samples, and CT answers the detailed questions about pore position, size and geometry. All three need agreed acceptance criteria per zone, a qualified procedure – and a casting process that keeps porosity low in the first place.

Frequently Asked Questions

Questions About X-Ray and CT Inspection of Die Castings

What Is the Difference Between Radiography and Radioscopy?

Radiography records single images; radioscopy produces live images while the part moves, suited to fast production inspection.

Does ASTM E505 Define Which Porosity Is Acceptable?

No. It shows categories and severity levels; the acceptable level is agreed between purchaser and manufacturer.

Can CT Replace a Leak Test?

Generally not. Leakage paths can be smaller than CT resolution; the leak test remains the functional proof.

How Small Can a Pore Be to Still Be Detected by CT?

It depends on voxel size and thus on the scanned size. A pore must cover several voxels; small parts or cut-outs allow much finer resolution.

Planning a Die Casting Cell?

Die Casting Machines from FISS.

Stable casting quality starts with the machine. FISS supplies used cold-chamber die casting machines and helps you choose the right equipment.

Sources

ASTM International: E505-22 Standard Reference Radiographs for Inspection of Aluminum and Magnesium Die Castings and E2973-22 Digital Reference Images for Inspection of Aluminum and Magnesium Die Castings, abstracts via store.astm.org and dinmedia.de, accessed 5 November 2026.

CEN: EN 12681-1:2017 Founding – Radiographic testing – Part 1: Film techniques and EN 12681-2:2017 Part 2: Techniques with digital detectors, scope summaries via standards catalogues, accessed 5 November 2026.

ISO: ISO 15708 Non-destructive testing – Radiation methods for computed tomography, Parts 1–4, catalogue entries iso.org, accessed 5 November 2026.

VDG/BDG: P 201, P 202 Volume deficits of castings made from aluminium, magnesium and zinc casting alloys (2010) and P 203 (CT porosity analysis, 2019), as described by DIN Media, Volume Graphics and QZ Qualität und Zuverlässigkeit 07/2021, accessed 5 November 2026.

ZEISS: 2D X-ray inspection systems and press release ZEISS OMNIA GC 220-180, 2025, zeiss.com, accessed 5 November 2026 (manufacturer statements).

DGUV: FAQ Röntgenanlage, stationäre (notification and licensing under the Radiation Protection Act), dguv.de, accessed 5 November 2026.